{"id":21108,"date":"2026-11-04T10:46:58","date_gmt":"2026-11-04T10:46:58","guid":{"rendered":"https:\/\/aludiecasting.com\/?p=21108"},"modified":"2026-11-04T10:46:58","modified_gmt":"2026-11-04T10:46:58","slug":"10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem","status":"publish","type":"post","link":"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/","title":{"rendered":"10 b\u011b\u017en\u00fdch vad p\u0159i gravita\u010dn\u00edm lit\u00ed hlin\u00edku do forem"},"content":{"rendered":"<p><a href=\"https:\/\/aludiecasting.com\/cs\/gravitacni-liti-hliniku-3\/\"><em><strong>Gravita\u010dn\u00ed tlakov\u00e9 lit\u00ed<\/strong><\/em><\/a> je jedn\u00edm z nejspolehliv\u011bj\u0161\u00edch zp\u016fsob\u016f v\u00fdroby kvalitn\u00edch a pevn\u00fdch hlin\u00edkov\u00fdch sou\u010d\u00e1st\u00ed \u2013 ale stejn\u011b jako ka\u017ed\u00fd odl\u00e9vac\u00ed proces m\u016f\u017ee v\u00e9st k vad\u00e1m, kter\u00e9 zp\u016fsobuj\u00ed pl\u00fdtv\u00e1n\u00ed kovem, \u010dasem i pen\u011bzi. Dobrou zpr\u00e1vou je, \u017ee t\u00e9m\u011b\u0159 ka\u017ed\u00e1 b\u011b\u017en\u00e1 vada m\u00e1 zn\u00e1mou p\u0159\u00ed\u010dinu a praktick\u00e9 preventivn\u00ed opat\u0159en\u00ed. Tato p\u0159\u00edru\u010dka vysv\u011btluje deset vad, s nimi\u017e se odb\u011bratel\u00e9 a in\u017een\u00fd\u0159i p\u0159i gravita\u010dn\u00edm lit\u00ed hlin\u00edku setk\u00e1vaj\u00ed nej\u010dast\u011bji, co je zp\u016fsobuje a jak\u00e9 konkr\u00e9tn\u00ed kroky podnik\u00e1 dob\u0159e funguj\u00edc\u00ed sl\u00e9v\u00e1rna, aby se jim vyhnula. Pokud hled\u00e1te dodavatele odlitk\u016f, znalost t\u011bchto pojm\u016f v\u00e1m pom\u016f\u017ee kl\u00e1st spr\u00e1vn\u00e9 ot\u00e1zky \u2013 a rozpoznat sl\u00e9v\u00e1rny, kter\u00e9 v\u011bd\u00ed, co d\u011blaj\u00ed.<\/p>\n<div id=\"ez-toc-container\" class=\"ez-toc-v2_0_91 counter-hierarchy ez-toc-counter ez-toc-grey ez-toc-container-direction\">\n<div class=\"ez-toc-title-container\">\n<p class=\"ez-toc-title\" style=\"cursor:inherit\">Obsah<\/p>\n<span class=\"ez-toc-title-toggle\"><a href=\"#\" class=\"ez-toc-pull-right ez-toc-btn ez-toc-btn-xs ez-toc-btn-default ez-toc-toggle\" aria-label=\"P\u0159epnut\u00ed tabulky obsahu\"><span class=\"ez-toc-js-icon-con\"><span class=\"\"><span class=\"eztoc-hide\" style=\"display:none;\">P\u0159ep\u00edna\u010d<\/span><span class=\"ez-toc-icon-toggle-span\"><svg style=\"fill: #7c7c7c;color:#7c7c7c\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\" class=\"list-377408\" width=\"20px\" height=\"20px\" viewbox=\"0 0 24 24\" fill=\"none\"><path d=\"M6 6H4v2h2V6zm14 0H8v2h12V6zM4 11h2v2H4v-2zm16 0H8v2h12v-2zM4 16h2v2H4v-2zm16 0H8v2h12v-2z\" fill=\"currentColor\"><\/path><\/svg><svg style=\"fill: #7c7c7c;color:#7c7c7c\" class=\"arrow-unsorted-368013\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\" width=\"10px\" height=\"10px\" viewbox=\"0 0 24 24\" version=\"1.2\" baseprofile=\"tiny\"><path d=\"M18.2 9.3l-6.2-6.3-6.2 6.3c-.2.2-.3.4-.3.7s.1.5.3.7c.2.2.4.3.7.3h11c.3 0 .5-.1.7-.3.2-.2.3-.5.3-.7s-.1-.5-.3-.7zM5.8 14.7l6.2 6.3 6.2-6.3c.2-.2.3-.5.3-.7s-.1-.5-.3-.7c-.2-.2-.4-.3-.7-.3h-11c-.3 0-.5.1-.7.3-.2.2-.3.5-.3.7s.1.5.3.7z\"\/><\/svg><\/span><\/span><\/span><\/a><\/span><\/div>\n<nav><ul class='ez-toc-list ez-toc-list-level-1' ><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-1\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#Why_Gravity_die_casting_Casting_Defects_Happen_Solidification_and_Feeding\" >Pro\u010d doch\u00e1z\u00ed k vad\u00e1m p\u0159i tlakov\u00e9m lit\u00ed metodou Gravity: tuhnut\u00ed a nap\u00e1jen\u00ed<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-2\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#1_Shrinkage_Porosity\" >1. Por\u00e9znost zp\u016fsoben\u00e1 smr\u0161t\u011bn\u00edm<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-3\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#2_Gas_Hydrogen_Porosity\" >2. Por\u00e9znost plynu (vod\u00edku)<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-4\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#3_Hot_Tearing\" >3. Trh\u00e1n\u00ed za tepla<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-5\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#4_Cold_Cracking\" >4. Prask\u00e1n\u00ed za studena<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-6\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#5_Non-Fills_Cold_Shuts_and_Misruns\" >5. Nevypln\u011bn\u00e9 m\u00edsta, studen\u00e9 spoje a vadn\u00e9 v\u00fdlisky<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-7\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#6_Oxide_and_Non-Metallic_Inclusions\" >6. Oxidov\u00e9 a nekovov\u00e9 vm\u011bstky<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-8\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#7_Segregation\" >7. Segregace<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-9\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#8_Iron_Intermetallics\" >8. Intermetalick\u00e9 slou\u010deniny \u017eeleza<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-10\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#9_Surface_and_Die-Related_Defects\" >9. Vady povrchu a vady souvisej\u00edc\u00ed s \u010dipem<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-11\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#10_Distortion_and_Dimensional_Variation\" >10. Deformace a rozm\u011brov\u00e9 odchylky<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-12\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#The_Cure_Directional_Solidification_Risers_and_Chills\" >\u0158e\u0161en\u00ed: sm\u011brov\u00e9 tuhnut\u00ed, v\u00fdstupky a chladic\u00ed kan\u00e1ly<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-13\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#Prevention_Checklist\" >Kontroln\u00ed seznam pro prevenci<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-14\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#Frequently_Asked_Questions\" >\u010casto kladen\u00e9 ot\u00e1zky<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-1'><a class=\"ez-toc-link ez-toc-heading-15\" href=\"https:\/\/aludiecasting.com\/cs\/10-beznych-vad-pri-gravitacnim-liti-hliniku-do-forem\/#Conclusion\" >Z\u00e1v\u011br<\/a><\/li><\/ul><\/nav><\/div>\n<h1><span class=\"ez-toc-section\" id=\"Why_Gravity_die_casting_Casting_Defects_Happen_Solidification_and_Feeding\"><\/span>Pro\u010d doch\u00e1z\u00ed k vad\u00e1m p\u0159i tlakov\u00e9m lit\u00ed metodou Gravity: tuhnut\u00ed a nap\u00e1jen\u00ed<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Hlin\u00edkov\u00e9 slitiny se p\u0159i p\u0159echodu z kapaln\u00e9ho do pevn\u00e9ho skupenstv\u00ed smr\u0161\u0165uj\u00ed p\u0159ibli\u017en\u011b o 3,5 % a\u017e 8,5 % objemu a p\u0159i ochlazov\u00e1n\u00ed pevn\u00e9ho kovu se d\u00e1le smr\u0161\u0165uj\u00ed. Kov, kter\u00fd vypl\u0148uje dutinu jako prvn\u00ed, proto mus\u00ed p\u0159ijmout dal\u0161\u00ed tekutinu, dokud je je\u0161t\u011b pastovit\u00fd \u2013 tomuto procesu se \u0159\u00edk\u00e1 pln\u011bn\u00ed. Pokud ur\u010dit\u00e1 oblast odlitku ztuhne d\u0159\u00edve, ne\u017e je zcela napln\u011bna, vznikne dutina. V\u011bt\u0161ina vad p\u0159i gravita\u010dn\u00edm odl\u00e9v\u00e1n\u00ed je jednodu\u0161e v\u00fdsledkem \u0161patn\u00e9 kontroly tuhnut\u00ed: teplo nen\u00ed odv\u00e1d\u011bno ve spr\u00e1vn\u00e9m po\u0159ad\u00ed, nebo konstrukce formy nedok\u00e1\u017ee dopravit kov na spr\u00e1vn\u00e9 m\u00edsto ve spr\u00e1vn\u00fd \u010das. Proto jsou nej\u00fa\u010dinn\u011bj\u0161\u00edmi preventivn\u00edmi n\u00e1stroji sm\u011brov\u00e9 tuhnut\u00ed, spr\u00e1vn\u011b dimenzovan\u00e9 napou\u0161t\u011bc\u00ed kan\u00e1ly a chladic\u00ed \u017el\u00e1bky \u2013 nikoli odhady p\u0159\u00edmo ve v\u00fdrob\u011b.<\/p>\n<p>Existuje u\u017eite\u010dn\u00fd zp\u016fsob, jak o tom uva\u017eovat. Vada, kterou lze vid\u011bt na povrchu, je \u010dasto viditeln\u00fdm projevem probl\u00e9mu, k n\u011bmu\u017e do\u0161lo ji\u017e d\u0159\u00edve, b\u011bhem taven\u00ed nebo tuhnut\u00ed. Drsn\u00fd povrch m\u016f\u017ee b\u00fdt zp\u016fsoben probl\u00e9mem s povrchovou \u00fapravou formy; por\u00e9zn\u00ed oblast, ze kter\u00e9 pod tlakem unik\u00e1 hmota, je obvykle zp\u016fsobena probl\u00e9mem s p\u0159\u00edvodem taveniny. Pokud sl\u00e9v\u00e1rna vede p\u0159esn\u00e9 z\u00e1znamy o teplot\u011b lit\u00ed, teplot\u011b formy a \u00faprav\u011b taveniny pro ka\u017edou s\u00e9rii, vady p\u0159est\u00e1vaj\u00ed b\u00fdt z\u00e1hadou a st\u00e1vaj\u00ed se vzorem, kter\u00fd lze odstranit.<\/p>\n<p><a href=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21076\" src=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum.jpg\" alt=\"forge and die cast aluminum\" width=\"1399\" height=\"756\" srcset=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum.jpg 1399w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum-1280x692.jpg 1280w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum-980x530.jpg 980w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2026\/10\/forge-and-die-cast-aluminum-480x259.jpg 480w\" sizes=\"(min-width: 0px) and (max-width: 480px) 480px, (min-width: 481px) and (max-width: 980px) 980px, (min-width: 981px) and (max-width: 1280px) 1280px, (min-width: 1281px) 1399px, 100vw\" \/><\/a><\/p>\n<h1><span class=\"ez-toc-section\" id=\"1_Shrinkage_Porosity\"><\/span>1. Por\u00e9znost zp\u016fsoben\u00e1 smr\u0161t\u011bn\u00edm<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Por\u00e9znost zp\u016fsoben\u00e1 smr\u0161\u0165ov\u00e1n\u00edm vznik\u00e1 v t\u011bch \u010d\u00e1stech odlitku, kter\u00e9 tuhnou jako posledn\u00ed \u2013 obvykle v siln\u00fdch \u010d\u00e1stech nebo \u201chork\u00fdch m\u00edstech\u201d \u2013, kam se tekut\u00fd kov nestihne dostat p\u0159ed dokon\u010den\u00edm tuhnut\u00ed. V\u00fdsledn\u00e9 dutiny maj\u00ed nepravideln\u00fd, drsn\u00fd a hranat\u00fd tvar. Oslabuj\u00ed danou \u010d\u00e1st a pod tlakem z nich m\u016f\u017ee unikat tekutina. Prevence spo\u010d\u00edv\u00e1 v \u0159\u00edzen\u00ed p\u0159\u00edvodu kovu a tepla: dimenzujte napou\u0161t\u011bc\u00ed kan\u00e1ly tak, aby z\u00e1sobovaly siln\u00e9 \u010d\u00e1sti, um\u00edst\u011bte chladic\u00ed prvky do hork\u00fdch m\u00edst, aby tam kov ztuhnul d\u0159\u00edve, udr\u017eujte rovnom\u011brnou tlou\u0161\u0165ku st\u011bny a navrhn\u011bte odlitek tak, aby tuhnul sm\u011brem k napou\u0161t\u011bc\u00edmu kan\u00e1lu. Simula\u010dn\u00ed software se dnes b\u011b\u017en\u011b pou\u017e\u00edv\u00e1 ke kontrole p\u0159\u00edvodu kovu je\u0161t\u011b p\u0159ed vyroben\u00edm formy.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"2_Gas_Hydrogen_Porosity\"><\/span>2. Por\u00e9znost plynu (vod\u00edku)<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Vod\u00edk je jedin\u00fd plyn, kter\u00fd se ve roztaven\u00e9m hlin\u00edku v\u00fdznamn\u011b rozpou\u0161t\u00ed, a jeho rozpustnost prudce kles\u00e1 p\u0159i tuhnut\u00ed kovu. Vytla\u010den\u00fd vod\u00edk vytv\u00e1\u0159\u00ed uvnit\u0159 odlitku zaoblen\u00e9 plynov\u00e9 p\u00f3ry. P\u00f3rovitost zp\u016fsoben\u00e1 plynem vznik\u00e1 v d\u016fsledku vlhkosti ve surovinov\u00e9 sm\u011bsi, vlhk\u00fdch tavidlech nebo vod\u00edku absorbovan\u00e9ho p\u0159i taven\u00ed. Prevence za\u010d\u00edn\u00e1 ji\u017e ve tavenin\u011b: odply\u0148ujte dus\u00edkem nebo argonem, udr\u017eujte surovinovou sm\u011bs \u010distou a suchou, vyh\u00fdbejte se nadm\u011brn\u00fdm teplot\u00e1m a prodlev\u00e1m a odl\u00e9vejte klidn\u011b, aby turbulence nevt\u00e1hla vzduch.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"3_Hot_Tearing\"><\/span>3. Trh\u00e1n\u00ed za tepla<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>K trh\u00e1n\u00ed za tepla (naz\u00fdvan\u00e9mu tak\u00e9 prask\u00e1n\u00ed za tepla) doch\u00e1z\u00ed b\u011bhem tuhnut\u00ed, kdy\u017e dendrity je\u0161t\u011b odd\u011bluje tenk\u00fd kapaln\u00fd film. Pokud se smr\u0161\u0165uj\u00edc\u00ed se odlitek nem\u016f\u017ee voln\u011b smr\u0161\u0165ovat, film se roztrhne pod\u00e9l hranic zrn a zanech\u00e1 nepravidelnou, zubatou trhlinu \u2013 obvykle v m\u00edstech s vysokou teplotou nebo tam, kde se pr\u016f\u0159ez n\u00e1hle m\u011bn\u00ed. Jedn\u00e1 se o jednu z nejv\u00edce frustruj\u00edc\u00edch vad, proto\u017ee se objevuje sporadicky. Prevence se zam\u011b\u0159uje jak na slo\u017een\u00ed slitiny, tak na konstrukci: pou\u017e\u00edvejte slitiny s lep\u0161\u00ed odolnost\u00ed proti trhlin\u00e1m za tepla (pom\u00e1h\u00e1 vy\u0161\u0161\u00ed obsah k\u0159em\u00edku), zjemn\u011bte zrno, p\u0159idejte zaoblen\u00ed a polom\u011bry v m\u00edstech zm\u011bn pr\u016f\u0159ezu, udr\u017eujte rovnom\u011brnou tlou\u0161\u0165ku st\u011bny, zajist\u011bte dostate\u010dn\u00e9 nap\u00e1jen\u00ed, pou\u017e\u00edvejte chladic\u00ed \u017el\u00e1bky a sni\u017ete omezen\u00ed pomoc\u00ed skl\u00e1dac\u00edch p\u00edskov\u00fdch jader. D\u016fle\u017eit\u00e1 je tak\u00e9 regulace teploty formy a teploty lit\u00ed.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"4_Cold_Cracking\"><\/span>4. Prask\u00e1n\u00ed za studena<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Trhliny vznikaj\u00edc\u00ed za studena se tvo\u0159\u00ed pod solidusem, kdy\u017e je kov ji\u017e zcela ztuhl\u00fd. D\u00edly jsou sice zcela ztuhl\u00e9, ale st\u00e1le se smr\u0161\u0165uj\u00ed; pokud jsou omezeny formou nebo jsou vyhozeny p\u0159\u00edli\u0161 brzy, mohou vysok\u00e1 zbytkov\u00e1 nap\u011bt\u00ed zp\u016fsobit vznik k\u0159ehk\u00e9 trhliny. Na rozd\u00edl od trhlin vznikaj\u00edc\u00edch za tepla proch\u00e1zej\u00ed trhliny vznikaj\u00edc\u00ed za studena ztuhl\u00fdm kovem. Prevence spo\u010d\u00edv\u00e1 p\u0159edev\u0161\u00edm v chlazen\u00ed a vyhazov\u00e1n\u00ed: nechte odlitek rovnom\u011brn\u011b vychladnout, upravte rozlo\u017een\u00ed teploty ve form\u011b, vyho\u010fte odlitek p\u0159i spr\u00e1vn\u00e9 teplot\u011b, vyhn\u011bte se ostr\u00fdm roh\u016fm, kter\u00e9 koncentruj\u00ed nap\u011bt\u00ed, a pou\u017eijte chladic\u00ed p\u0159\u00edpravky k podep\u0159en\u00ed d\u00edlu b\u011bhem chlazen\u00ed.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"5_Non-Fills_Cold_Shuts_and_Misruns\"><\/span>5. Nevypln\u011bn\u00e9 m\u00edsta, studen\u00e9 spoje a vadn\u00e9 v\u00fdlisky<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Jedn\u00e1 se o vady vypln\u011bn\u00ed, p\u0159i nich\u017e roztaven\u00fd kov ztuhne d\u0159\u00edve, ne\u017e zcela vypln\u00ed dutinu. \u201eCold shut\u201c je viditeln\u00fd \u0161ev, kde se dva proudy kovu nespojily; \u201emisrun\u201c je ne\u00fapln\u00e1 \u010d\u00e1st v\u00fdlisk\u016f. Jsou zp\u016fsobeny p\u0159\u00edli\u0161 chladn\u00fdm lit\u00edm, tenk\u00fdmi st\u011bnami, kter\u00e9 kov ochlazuj\u00ed p\u0159\u00edli\u0161 rychle, \u0161patnou tekutost\u00ed slitiny, p\u0159\u00edli\u0161 chladnou formou nebo nevhodn\u00fdm vtokov\u00fdm syst\u00e9mem. Prevenci zaji\u0161\u0165uje regulace teploty lit\u00ed, p\u0159edeh\u0159\u00e1t\u00ed formy na spr\u00e1vnou pracovn\u00ed teplotu, n\u00e1vrh vtok\u016f, kter\u00e9 nejprve vypln\u00ed tenk\u00e9 \u010d\u00e1sti, a volba slitin s dobrou tekutost\u00ed.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"6_Oxide_and_Non-Metallic_Inclusions\"><\/span>6. Oxidov\u00e9 a nekovov\u00e9 vm\u011bstky<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Hlin\u00edk okam\u017eit\u011b reaguje s kysl\u00edkem, tak\u017ee na povrchu taveniny se v\u017edy vyskytuj\u00ed oxidov\u00e9 vrstvy a struska. Pokud se tyto l\u00e1tky dostanou do odlitku \u2013 v d\u016fsledku turbulentn\u00edho lit\u00ed, nedostate\u010dn\u00e9ho odstra\u0148ov\u00e1n\u00ed strusky nebo zne\u010di\u0161t\u011bn\u00e9 taveniny \u2013 vzniknou z nich nekovov\u00e9 vm\u011bstky, kter\u00e9 oslabuj\u00ed d\u00edl a ni\u010d\u00ed obroben\u00e9 nebo eloxovan\u00e9 povrchy. Prevenc\u00ed je d\u016fsledn\u00e1 manipulace s taveninou: spr\u00e1vn\u00e9 odstra\u0148ov\u00e1n\u00ed strusky a tavidla, odply\u0148ov\u00e1n\u00ed, filtrov\u00e1n\u00ed kovu v m\u00edst\u011b lit\u00ed, klidn\u00e9 a rovnom\u011brn\u00e9 lit\u00ed a udr\u017eov\u00e1n\u00ed taveniny bez nahromad\u011bn\u00e9 strusky.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"7_Segregation\"><\/span>7. Segregace<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Segregace je lok\u00e1ln\u00ed zm\u011bna chemick\u00e9ho slo\u017een\u00ed v odlitku, nej\u010dast\u011bji se jedn\u00e1 o \u201cinverzn\u00ed segregaci\u201d, p\u0159i n\u00ed\u017e je posledn\u00ed kapaln\u00e1 f\u00e1ze bohat\u00e1 na eutektikum vytla\u010dov\u00e1na sm\u011brem k povrchu nebo do oblast\u00ed nap\u00e1jec\u00edch kan\u00e1lk\u016f. To zp\u016fsobuje nerovnom\u011brn\u00e9 mechanick\u00e9 vlastnosti a nejednotnou reakci na tepeln\u00e9 zpracov\u00e1n\u00ed. Je \u0159\u00edzena podm\u00ednkami tuhnut\u00ed a v p\u0159\u00edpad\u011b pot\u0159eby tak\u00e9 homogeniza\u010dn\u00edm \u017e\u00edh\u00e1n\u00edm (dif\u00faze popsan\u00e1 Fickov\u00fdm z\u00e1konem) po odlit\u00ed, kter\u00e9 m\u00e1 za c\u00edl vyrovnat slo\u017een\u00ed. Sl\u00e9v\u00e1rny, kter\u00e9 p\u0159\u00edsn\u011b kontroluj\u00ed chlazen\u00ed a povlakov\u00e1n\u00ed forem, se s v\u00fdznamnou segregac\u00ed setk\u00e1vaj\u00ed jen z\u0159\u00eddka.<\/p>\n<div id=\"attachment_13246\" style=\"width: 337px\" class=\"wp-caption aligncenter\"><a href=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2019\/09\/Gravity-die-casting.jpg\"><img loading=\"lazy\" decoding=\"async\" aria-describedby=\"caption-attachment-13246\" class=\"wp-image-13246 size-full\" src=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2019\/09\/Gravity-die-casting.jpg\" alt=\"Gravity die casting defects\" width=\"327\" height=\"351\" srcset=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2019\/09\/Gravity-die-casting.jpg 327w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2019\/09\/Gravity-die-casting-279x300.jpg 279w\" sizes=\"(max-width: 327px) 100vw, 327px\" \/><\/a><p id=\"caption-attachment-13246\" class=\"wp-caption-text\">Gravita\u010dn\u00ed tlakov\u00e9 lit\u00ed<\/p><\/div>\n<h1><span class=\"ez-toc-section\" id=\"8_Iron_Intermetallics\"><\/span>8. Intermetalick\u00e9 slou\u010deniny \u017eeleza<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>\u017delezo se \u010dasto vyskytuje v sekund\u00e1rn\u00edch hlin\u00edkov\u00fdch slitin\u00e1ch, kde tvo\u0159\u00ed jehlicovit\u00e9 f\u00e1ze \u03b2-AlFeSi, kter\u00e9 jsou tvrd\u00e9 a k\u0159ehk\u00e9. Sni\u017euj\u00ed ta\u017enost, zkracuj\u00ed \u00fanavovou \u017eivotnost a podporuj\u00ed vznik mikroporozity zp\u016fsoben\u00e9 smr\u0161\u0165ov\u00e1n\u00edm. Vzhledem k tomu, \u017ee \u017eelezo je obt\u00ed\u017en\u00e9 z taveniny odstranit, je t\u0159eba se zam\u011b\u0159it na prevenci z metalurgick\u00e9ho hlediska: pro n\u00e1ro\u010dn\u00e9 d\u00edly je t\u0159eba specifikovat slitiny s n\u00edzk\u00fdm obsahem \u017eeleza, p\u0159idat mangan, aby se k\u0159ehk\u00e1 \u03b2-f\u00e1ze p\u0159em\u011bnila na m\u00e9n\u011b \u0161kodlivou \u03b1-f\u00e1zi, a pou\u017e\u00edt rychlej\u0161\u00ed ochlazov\u00e1n\u00ed, aby \u0161kodliv\u00e9 jehlicovit\u00e9 \u00fatvary z\u016fstaly mal\u00e9.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"9_Surface_and_Die-Related_Defects\"><\/span>9. Vady povrchu a vady souvisej\u00edc\u00ed s \u010dipem<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Hrub\u00e9 povrchy, p\u0159ip\u00e1jen\u00ed, ulp\u00edv\u00e1n\u00ed a ot\u0159epy jsou obvykle p\u0159\u00edznaky stavu formy, nikoli slitiny. Pokud je povlak formy opot\u0159ebovan\u00fd, je nespr\u00e1vn\u00e1 pracovn\u00ed teplota nebo do\u0161lo k erozi povrchu formy, trp\u00ed t\u00edm povrch odlitku a d\u00edly se lep\u00ed. Prevenc\u00ed je d\u016fsledn\u00e1 \u00fadr\u017eba n\u00e1stroj\u016f: v\u010dasn\u00e9 obnoven\u00ed \u017e\u00e1ruvzdorn\u00e9ho povlaku, kontrola pracovn\u00ed teploty formy, kontrola eroze a vym\u00fdv\u00e1n\u00ed a pou\u017eit\u00ed vhodn\u00e9ho uvol\u0148ovac\u00edho prost\u0159edku. \u010cist\u00e1 a dob\u0159e udr\u017eovan\u00e1 forma je nejlevn\u011bj\u0161\u00ed pojistkou proti povrchov\u00fdm vad\u00e1m.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"10_Distortion_and_Dimensional_Variation\"><\/span>10. Deformace a rozm\u011brov\u00e9 odchylky<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Tenk\u00e9 nebo asymetrick\u00e9 \u010d\u00e1sti chladnou r\u016fznou rychlost\u00ed a v\u00fdsledn\u00e9 zbytkov\u00e9 nap\u011bt\u00ed zp\u016fsobuje deformaci d\u00edlu nebo jeho posun mimo toleran\u010dn\u00ed rozmez\u00ed. Prevence spo\u010d\u00edv\u00e1 v rovnom\u011brn\u00e9m ochlazov\u00e1n\u00ed: vyv\u00e1\u017een\u00ed tlou\u0161\u0165ky st\u011bny, \u0159\u00edzen\u00ed rozlo\u017een\u00ed teploty ve form\u011b, rovnom\u011brn\u00e9 ochlazov\u00e1n\u00ed d\u00edlu, vyjmut\u00ed p\u0159i spr\u00e1vn\u00e9 teplot\u011b a pou\u017eit\u00ed chladic\u00edch p\u0159\u00edpravk\u016f k udr\u017een\u00ed tvaru b\u011bhem tuhnut\u00ed odlitku. \u010c\u00edm d\u0159\u00edve se t\u00edmto probl\u00e9mem zab\u00fdv\u00e1te v procesu n\u00e1vrhu, t\u00edm m\u00e9n\u011b p\u0159ekvapen\u00ed se objev\u00ed ve v\u00fdrob\u011b.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"The_Cure_Directional_Solidification_Risers_and_Chills\"><\/span>\u0158e\u0161en\u00ed: sm\u011brov\u00e9 tuhnut\u00ed, v\u00fdstupky a chladic\u00ed kan\u00e1ly<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Za v\u011bt\u0161inou t\u011bchto vad stoj\u00ed jedna z\u00e1sada: odlitek by m\u011bl tuhnout od nejten\u010d\u00edho m\u00edsta sm\u011brem k nejtlust\u0161\u00edmu a napou\u0161t\u011bc\u00ed kan\u00e1l \u2013 oblast, kter\u00e1 tuhne jako posledn\u00ed \u2013 by m\u011bl odlitek z\u00e1sobovat a\u017e do \u00fapln\u00e9ho ztuhnut\u00ed. Jedn\u00e1 se o sm\u011brov\u00e9 tuhnut\u00ed. Velikost vtok\u016f se ur\u010duje metodou modulu: u odlitk\u016f z ne\u017eelezn\u00fdch kov\u016f je modul vtoku obvykle asi 1,3 a\u017e 1,4n\u00e1sobkem modulu profilu, kter\u00fd z\u00e1sobuje. Chladi\u010de, obvykle m\u011bd\u011bn\u00e9 nebo \u017eelezn\u00e9 bloky um\u00edst\u011bn\u00e9 ve form\u011b proti siln\u00fdm \u010d\u00e1stem, urychluj\u00ed lok\u00e1ln\u00ed ochlazov\u00e1n\u00ed, tak\u017ee hork\u00e9 m\u00edsto ztuhne d\u0159\u00edve, m\u00edsto aby doch\u00e1zelo k nedostate\u010dn\u00e9mu p\u0159\u00edsunu kovu.<\/p>\n<p><a href=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2023\/10\/Untitled-design-12-1.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-14610\" src=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2023\/10\/Untitled-design-12-1.jpg\" alt=\"Gravita\u010dn\u00ed lit\u00ed hlin\u00edku\" width=\"1000\" height=\"600\" srcset=\"https:\/\/aludiecasting.com\/wp-content\/uploads\/2023\/10\/Untitled-design-12-1.jpg 1000w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2023\/10\/Untitled-design-12-1-980x588.jpg 980w, https:\/\/aludiecasting.com\/wp-content\/uploads\/2023\/10\/Untitled-design-12-1-480x288.jpg 480w\" sizes=\"(min-width: 0px) and (max-width: 480px) 480px, (min-width: 481px) and (max-width: 980px) 980px, (min-width: 981px) 1000px, 100vw\" \/><\/a><\/p>\n<p>Celkov\u00fd obraz dopl\u0148uj\u00ed dva faktory z v\u00fdrobn\u00ed linky: pracovn\u00ed teplota formy a zp\u016fsob jej\u00edho povlakov\u00e1n\u00ed. P\u0159\u00edli\u0161 studen\u00e1 forma zp\u016fsobuje vznik studen\u00fdch \u0161v\u016f a plynovou por\u00e9znost, zat\u00edmco p\u0159\u00edli\u0161 hork\u00e1 forma zpomaluje tuhnut\u00ed a zhor\u0161uje smr\u0161\u0165ov\u00e1n\u00ed. \u017d\u00e1ruvzdorn\u00fd povlak formy nen\u00ed pouhou ozdobou \u2013 \u0159\u00edd\u00ed, jak rychle teplo opou\u0161t\u00ed kov a uvol\u0148uje hotov\u00fd d\u00edl. Sl\u00e9v\u00e1rny, kter\u00e9 pova\u017euj\u00ed teplotu formy a jej\u00ed povlak za procesn\u00ed parametry a sleduj\u00ed je v ka\u017ed\u00e9 sm\u011bn\u011b, maj\u00ed trvale ni\u017e\u0161\u00ed m\u00edru vad ne\u017e ty, kter\u00e9 je ponech\u00e1vaj\u00ed n\u00e1hod\u011b.<\/p>\n<table style=\"width: 598px;\">\n<thead>\n<tr>\n<td style=\"width: 114.389px;\"><strong>N\u00e1stroj<\/strong><\/td>\n<td style=\"width: 237.042px;\"><strong>Jak to funguje<\/strong><\/td>\n<td style=\"width: 226.347px;\"><strong>Poruchy, kter\u00fdm zabra\u0148uje<\/strong><\/td>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"width: 114.389px;\">Stoupa\u010dky<\/td>\n<td style=\"width: 237.042px;\">Uchov\u00e1vejte tekut\u00fd kov a p\u0159iv\u00e1d\u011bjte jej do odlitku, dokud neztuhne<\/td>\n<td style=\"width: 226.347px;\">Por\u00e9znost zp\u016fsoben\u00e1 smr\u0161t\u011bn\u00edm, trh\u00e1n\u00ed za tepla<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 114.389px;\">Zimnice<\/td>\n<td style=\"width: 237.042px;\">Zrychlit lok\u00e1ln\u00ed chlazen\u00ed u siln\u00fdch profil\u016f<\/td>\n<td style=\"width: 226.347px;\">Por\u00e9znost zp\u016fsoben\u00e1 smr\u0161t\u011bn\u00edm, trh\u00e1n\u00ed za tepla<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 114.389px;\">P\u00edskov\u00e1 j\u00e1dra<\/td>\n<td style=\"width: 237.042px;\">Vytvo\u0159te vnit\u0159n\u00ed pr\u016fchody a umo\u017en\u011bte kontrakci<\/td>\n<td style=\"width: 226.347px;\">Trh\u00e1n\u00ed za tepla, deformace<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 114.389px;\">Povlakov\u00e1n\u00ed forem<\/td>\n<td style=\"width: 237.042px;\">Upravte odvod tepla a uvoln\u011bte d\u00edl<\/td>\n<td style=\"width: 226.347px;\">Povrchov\u00e9 vady, slepen\u00ed, studen\u00e9 svary<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 114.389px;\">Simulace (FEM)<\/td>\n<td style=\"width: 237.042px;\">P\u0159ed v\u00fdrobou n\u00e1stroj\u016f zkontrolujte konstrukci vtok\u016f a v\u00fdtok\u016f<\/td>\n<td style=\"width: 226.347px;\">V\u0161echny vady v pln\u011bn\u00ed a p\u00f3rovitosti<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h1><span class=\"ez-toc-section\" id=\"Prevention_Checklist\"><\/span>Kontroln\u00ed seznam pro prevenci<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>Sl\u00e9v\u00e1rna, kter\u00e1 trvale vyr\u00e1b\u00ed bezvadn\u00e9 odlitky gravita\u010dn\u00edm odl\u00e9v\u00e1n\u00edm, se obvykle \u0159\u00edd\u00ed kontroln\u00edm seznamem, jako je tento. Pokud odlitky nakupujete, pr\u00e1v\u011b tyto ot\u00e1zky stoj\u00ed za to polo\u017eit.<\/p>\n<table>\n<thead>\n<tr>\n<td width=\"159\"><strong>Defekt<\/strong><\/td>\n<td width=\"370\"><strong>Kl\u00ed\u010dov\u00e1 preventivn\u00ed opat\u0159en\u00ed<\/strong><\/td>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td width=\"159\">Smr\u0161\u0165ovac\u00ed p\u00f3rovitost<\/td>\n<td width=\"370\">Spr\u00e1vn\u00e1 velikost stoupac\u00edho kan\u00e1lu; ochlazov\u00e1n\u00ed v m\u00edstech s vysokou teplotou; sm\u011brov\u00e9 tuhnut\u00ed; rovnom\u011brn\u00e1 tlou\u0161\u0165ka st\u011bny<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">P\u00f3rovitost plynu<\/td>\n<td width=\"370\">Degas (N\u2082\/Ar); such\u00e1, \u010dist\u00e1 n\u00e1pl\u0148; regulovan\u00e1 teplota; klidn\u00e9 nal\u00e9v\u00e1n\u00ed<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Hot tearing<\/td>\n<td width=\"370\">Hot-tear-resistant alloy; grain refinement; radii at transitions; chills; collapsible cores; adequate feeding<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Cold cracking<\/td>\n<td width=\"370\">Even cooling; correct ejection temperature; cooling fixtures; avoid stress raisers<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Non-fills \/ cold shuts<\/td>\n<td width=\"370\">Correct pouring temperature; preheat the die; good gating; fluid alloy<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Oxide inclusions<\/td>\n<td width=\"370\">Skim and flux; filter; quiescent pouring; clean melt<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Segregation<\/td>\n<td width=\"370\">Controlled solidification; mould coating; homogenisation anneal if needed<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Iron intermetallics<\/td>\n<td width=\"370\">Low-iron alloy; manganese addition; faster cooling<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Surface \/ die defects<\/td>\n<td width=\"370\">Die coating on schedule; controlled die temperature; die inspection and maintenance<\/td>\n<\/tr>\n<tr>\n<td width=\"159\">Zkreslen\u00ed<\/td>\n<td width=\"370\">Balanced wall thickness; uniform die temperature; cooling fixtures<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h1><span class=\"ez-toc-section\" id=\"Frequently_Asked_Questions\"><\/span>\u010casto kladen\u00e9 ot\u00e1zky<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p><strong>What is the most common defect in <a href=\"https:\/\/www.thediecasting.com\/what-is-gravity-die-casting\/\" target=\"_blank\" rel=\"noopener\">gravita\u010dn\u00ed lit\u00ed hlin\u00edku<\/a>?<\/strong><\/p>\n<p>Shrinkage porosity is the most common and the most controllable. It is caused by insufficient feeding of the last regions to solidify and is prevented with correctly sized risers, chills and directional solidification.<\/p>\n<p><strong>Can gas porosity be removed from gravity castings?<\/strong><\/p>\n<p>Yes, mostly at the melt stage \u2014 degassing with nitrogen or argon removes hydrogen, and clean, dry handling prevents it returning. Castings can also be inspected by X-ray or pressure testing to confirm soundness.<\/p>\n<p><strong>Why do hot tears keep appearing even in a &#8220;good&#8221; die?<\/strong><\/p>\n<p>Hot tearing is strongly influenced by alloy composition, section geometry and restraint. A die that is otherwise fine can tear if the alloy has low hot-tear resistance, the section changes too abruptly, or a rigid core restricts contraction. Grain refinement, fillets, chills and collapsible cores are the usual fixes.<\/p>\n<p><strong>How can I check a supplier actually prevents defects?<\/strong><\/p>\n<p>Ask about their melt treatment (degassing, filtration), their die maintenance and coating schedule, whether they use risers and chills designed by the modulus method, and whether they run simulation or X-ray inspection. A supplier who can answer these in detail is far less likely to ship defective parts.<\/p>\n<p><strong>Does heat treatment fix casting defects?<\/strong><\/p>\n<p>Heat treatment can relieve stress and improve mechanical properties, but it cannot remove porosity, cracks or inclusions. Prevention at melting and solidification is the only real cure.<\/p>\n<h1><span class=\"ez-toc-section\" id=\"Conclusion\"><\/span>Z\u00e1v\u011br<span class=\"ez-toc-section-end\"><\/span><\/h1>\n<p>The defects that plague <em><strong>aluminium gravity die castings<\/strong><\/em> are neither mysterious nor unavoidable. Each one points back to a specific cause \u2014 usually a feeding problem, a melting problem, a mould condition, or a cooling issue \u2014 and each has a proven remedy. The best foundries combine careful melt treatment with sound riser and chill design, disciplined die maintenance, and simulation before the die is ever built. If you understand these ten defects and how they are prevented, you will be able to buy castings with far more confidence \u2014 and hold your suppliers to a higher standard.<\/p>","protected":false},"excerpt":{"rendered":"<p>Gravity die casting is one of the most reliable ways to produce sound, strong aluminium components \u2014 but like any casting process, it can throw up defects that waste metal, time and money. The good news is that almost every common defect has a known cause and a practical prevention. This guide explains the ten [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":15209,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"_et_pb_use_builder":"","_et_pb_old_content":"","_et_gb_content_width":"","footnotes":""},"categories":[1],"tags":[1350,1353],"class_list":["post-21108","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-aluminium-alloy-castings","tag-gravity-die-casting","tag-gravity-die-casting-defects"],"_links":{"self":[{"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/posts\/21108","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/comments?post=21108"}],"version-history":[{"count":3,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/posts\/21108\/revisions"}],"predecessor-version":[{"id":21113,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/posts\/21108\/revisions\/21113"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/media\/15209"}],"wp:attachment":[{"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/media?parent=21108"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/categories?post=21108"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/aludiecasting.com\/cs\/wp-json\/wp\/v2\/tags?post=21108"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}